Metal Dusting​

Metal dusting, also known as carbon attack, carbon rot, or catastrophic carburization, is a problem that often occurs in heat-treat carburizing furnaces and in petrochemical equipment.

RA330® Radiant Tube, used in 1650°F (900°C) carburizing service. The tube succumbed to metal dusting after 1 year.
RA330® Plate Welded with Alloy 82 (ERNiCr-3), in service at 1700°F (927°C) with a high carbon potential. Alloy 82 weld bead was locally attacked.

When this phenomenon occurs, the metal undergoes a destructive process that causes it to effectively disappear. What remains are either small, localized areas that appear to have been chewed away or large perforations. There are two temperature ranges in which metal dusting may occur. Typically, an operating temperature between 800 – 1200°F (430 -650°C) is where metal dusting takes place in stagnant areas in or near the furnace walls. A carburizing furnace usually operates at around 1750°F (950°C). However, some lower-temperature locations like alloy tube hangers, atmosphere sampling tubes, or where electrical leads pass through furnace walls where the atmosphere is stagnant, is where metal dusting could potentially occur. Occasionally, a higher temperature metal dusting may occur near 1650 – 1700°F (900 – 930°C), causing the metal to become thin or pitted. The pits at this higher temperature are close to 3/8” (10mm) in diameter in contrast to the roughly 1/8” (3mm) at the lower temperature.

In carburizing furnaces the atmosphere is a rich endothermic environment, with about 39% N­­2, 19.8% CO, 40% H2, 0.2% H2O, and 0.5% CH4. CO2 is low, about 0.1%. Metal dusting changes from aggravation to a significant economic matter as carbon potential increases to about 1% C or more. Metal dusting attacks have been identified in various industries, including hydrogen plant reformers, ammonia plant waste heat recovery boilers, syngas units, coal gasification reduction furnaces, heat treating furnaces, and direct reduced iron ore plants.

The resistance of an alloy to metal dusting has been linked to its ability to form a protective oxide scale even in low oxygen atmospheres that lead to metal dusting. As a result, alloys high in oxide formers tend to provide the greatest level of metal dusting resistance. Chromium, aluminum, and silicon are the most notable oxide forming elements in heat-resistant alloys. A widely accepted way of ranking the resistance of alloys to metal dusting is by calculating the chromium equivalent of the alloy. Generally, alloys with a chromium equivalent of 25 or greater offer moderate resistance to metal dusting, whereas alloys with greater chromium equivalents exceeding 30 are considered to have excellent resistance to metal dusting. Rolled Alloys offers many alloys that have been used to combat metal dusting such as RA602CA®, RA333®, and 625.

5-axis waterjet bevel cutting examples, including tapered and angled edges, precision holes, and clean cuts on metal parts.

5-Axis Waterjet Beveling

A 5-axis waterjet cutting machine is an advanced CNC cutting tool that uses a high-pressure stream of water mixed with abrasive (usually garnet) to cut

READ MORE

2026 Trade Show Schedule

Connect with our team in person throughout 2026 at these key industry events. Explore our full trade show schedule to discover where we’ll be exhibiting

READ MORE
Never Miss an Update - Subscribe Today!
Get application insights, material guides, and technical answers straight from the leaders in high-performance alloys.​

Share:

QUOTE, BUY, TRACK

We make it easy to get instant pricing and purchase your metal at the click of a button. Track your order progress, get notified when it ships, and follow your shipment online until it’s delivered. It’s that easy!

Latest Articles

5-Axis Waterjet Beveling

A 5-axis waterjet cutting machine is an advanced CNC cutting tool that uses a high-pressure stream of water mixed with abrasive (usually garnet) to cut through metals and other materials.

Read More »
2026 Trade Show Schedule

Connect with our team in person throughout 2026 at these key industry events. Explore our full trade show schedule to discover where we’ll be exhibiting all year long.

Read More »
How Titanium Sponge and Scrap Become Final Products

Titanium sponge and scrap are the starting materials for producing titanium ingots and slabs. Through processes like vacuum arc remelting (VAR) and hearth melting, these materials are refined into high-purity forms that are then forged, rolled, and finished into titanium plates, bars, and components.

Read More »
Alloying Elements Explained

Alloying elements play a critical role in shaping the strength, corrosion resistance, and performance of metals. This article breaks down the most common alloying elements, explains how they affect material properties, and provides guidance for choosing the right alloy for any application.

Read More »
Privacy Overview

This website uses cookies so that we can provide you with the best user experience possible. Cookie information is stored in your browser and performs functions such as recognising you when you return to our website and helping our team to understand which sections of the website you find most interesting and useful.