Ferrite Content in Austenitic Stainless Steels

The basic 300 series stainless steels like 304/304L and 316/316L have an austenitic microstructure and are non-magnetic. In the annealed condition, they are essentially free of ferrite, which is magnetic.

Cast products of these alloys typically have some ferrite present. These alloys also form some ferrite when they are cold-worked or work-hardened. In both cases, the products will show a magnetic tendency. Ferrite can be detrimental to corrosion resistance in some environments. There are also applications where magnetic characteristics interfere with a product’s performance.

The ferrite content of a cast alloy can be controlled through alloy composition. Carbon, nitrogen, nickel, and manganese are strong austenite formers, and increasing their content in the alloy will reduce the tendency for ferrite formation. There are several different methods of predicting ferrite content, one of the more common is by utilizing the DeLong diagram. Ferrite reduces the tendency for the steel to solidification crack during cooling. It is common for 304 castings (CF8) to contain 8-20% ferrite. The cast ingot composition of wrought 304/304L stainless is also balanced to have 1-6% ferrite since this reduces the chance of cracking during forging or hot working.

Calculate the nickel and chromium equivalents from the weld metal analysis. If nitrogen analysis of the weld is not available, assume 0.06% for GTA and covered electrode, or 0.08% for GMA weld metals. If the chemistry is accurate the diagram predicts the WRC Ferrite Number within plus or minus 3 in approximately 90% of the tests for 308, 309, 316 and 317 families.

Solution annealing will dissolve most of the ferrite retained from ingot solidification. Because cast products are balanced to have a higher amount of ferrite, annealing will not transform all of it into austenite. However, little or no ferrite will remain in an annealed wrought product.
The DeLong diagram also predicts the amount of ferrite likely to be present in a weld deposit made from the wrought product. Plotting the composition of the wrought plate or bar product will indicate how much ferrite might be present if the material were re-melted (i.e., welding). Still, it is not a valid indicator of the ferrite content in the annealed product. Ferrite content in the actual product can be determined through laborious metallographic examination or by using sensitive magnetic instruments in a laboratory setting (magnetic permeability). However, in most cases, comparative calibrated magnets can establish an approximate ferrite content within 0.5 – 1%. Standard annealed 304/304L, 316/316L, 309, and 310 testing tends to yield 2% or less values. Often, ferrite contents are less than 0.5%.

It should also be noted that the matching filler metals used to join these alloys will also have higher ferrite contents. This is a precaution against solidification cracking during welding.

Depending on the alloy, the ferrite contents in the weld deposits will be between 5 – 10% ferrite. If ferrite-free welds are required, a higher nickel alloy filler should be selected, such as Alloy 20 (ER320LR) or Alloy 625 (ERNiCrMo-3).

Please contact the Rolled Alloys Metallurgical Services group at 1-800-521-0332 or submit your questions below. 

5-axis waterjet bevel cutting examples, including tapered and angled edges, precision holes, and clean cuts on metal parts.

5-Axis Waterjet Beveling

A 5-axis waterjet cutting machine is an advanced CNC cutting tool that uses a high-pressure stream of water mixed with abrasive (usually garnet) to cut

READ MORE

2026 Trade Show Schedule

Connect with our team in person throughout 2026 at these key industry events. Explore our full trade show schedule to discover where we’ll be exhibiting

READ MORE
Never Miss an Update - Subscribe Today!
Get application insights, material guides, and technical answers straight from the leaders in high-performance alloys.​

Share:

QUOTE, BUY, TRACK

We make it easy to get instant pricing and purchase your metal at the click of a button. Track your order progress, get notified when it ships, and follow your shipment online until it’s delivered. It’s that easy!

Latest Articles

5-Axis Waterjet Beveling

A 5-axis waterjet cutting machine is an advanced CNC cutting tool that uses a high-pressure stream of water mixed with abrasive (usually garnet) to cut through metals and other materials.

Read More »
2026 Trade Show Schedule

Connect with our team in person throughout 2026 at these key industry events. Explore our full trade show schedule to discover where we’ll be exhibiting all year long.

Read More »
How Titanium Sponge and Scrap Become Final Products

Titanium sponge and scrap are the starting materials for producing titanium ingots and slabs. Through processes like vacuum arc remelting (VAR) and hearth melting, these materials are refined into high-purity forms that are then forged, rolled, and finished into titanium plates, bars, and components.

Read More »
Alloying Elements Explained

Alloying elements play a critical role in shaping the strength, corrosion resistance, and performance of metals. This article breaks down the most common alloying elements, explains how they affect material properties, and provides guidance for choosing the right alloy for any application.

Read More »
Privacy Overview

This website uses cookies so that we can provide you with the best user experience possible. Cookie information is stored in your browser and performs functions such as recognising you when you return to our website and helping our team to understand which sections of the website you find most interesting and useful.